COPPER.

435

The following statement will show the results ofOp. II:—

Substances Employed.

Calcined ore... 0.724

Crude ore . 0.084

Poor scoria, from Op. IV. 0.085

„ „ V. 0.051

„ „ VII. 0.008

Fluoride of calcium. 0.041

Earthy matters:—sand . 0.001

„ „ brick. 0.006

1.000

Products.

Coarse metal, for Op. III. .. 0.275

Scoria . 0.650

Furnace waste, from Op. IV. 0.009

Sulphurous acid . 0.055

Sublimed sulphur. 0.001

Fluoride of silicium. 0.008

Water and carbonic acid. 0.002

1.000

An examination of the scoria produced in Op. II.will always show whether the metal calciner men havedone their duty. The scoria are inspected in a court-yard, yy, Pig. 620, where the men deposit it in regularorder, under the number of each furnace. Each brickis broken with a hammer, and the fracture examined;the lower part of the brick is minutely inspected,especially that of the brick No. 1: the small grains ofmatt, mechanically mixed with the slag, exhibit a clearbronze colour, and a metallic lustre on the black, dullsurface of the fracture. The value of the copper inthe slags is thus judged of very accurately: if theproportion he from 3 -^, to an experienced eyecan tell within or the quantity of coppercontained therein. In breaking up the bricks theinspector forms the fragments into two heaps; thelarger heap contains those which are to be thrownupon the rubbish heap, r, Pig. 620, the other heapcontains those fragments which are to be returned tothe furnace. Each new charge contains 0.071 tonsof this rich scoria; a larger proportion than this wouldbe injurious, hut as a larger quantity than can beused is produced, the surplus is melted down oncea-week or fortnight, for which service the men receiveno pay.

The iron cylinder containing the coarse metal , as it iscalled, produced by two contiguous furnaces, is hauledup by means of a crane, Pig. 618, and conveyed inwheelbarrows to the depot, Pig. 620.

Sunday is to the men engaged in Op. I. and II.,what it ought to be to every one, a day of rest fromworldly occupation. The fires, however, require tobe kept up, and this service is performed by one man,who has the charge of 4 furnaces, and he must soarrange that the furnaces be at the f ull heat for thereception of the charges on Monday morning at 5o’clock.

Third Operation. —The coarse metal obtained inthe last operation is in very small fragments, externallyof a deep brown colour; they are easily crushed by ablow, and the surface of the fracture is of a brownishred. The metallic copper forms about -|d of the totalweight; it is, in fact, very similar to copper pyritesfree from gangue. It is, therefore, in the first partof Op. III. simply calcined with access of atmospheric

air. The charge is weighed out, and conveyed inwheelbarrows to the hoppers over the calcining fur-naces, which are similar to those used in Op. I. Eachof these is served by two men, who relieve each otheralternately. One man must work on Sunday, becauseeach operation extends over a period of 36 hours.

The most important part of this operation consists inthe management of the fire; it is the same in principleas in Op. I., but more fuel is consumed, and the heatrequires to be greatly increased towards the end ofthe operation; 0.043 tons of coal per hour is burnt,whereas in Op. I. it was only 0.035 tons. The chargehaving been spread over the sole, the temperature iskept up to the highest that it will bear without fusing.Two hours after the doors have been closed it emitsabundant fumes of sulphurous acid, and it is rabbledevery two hours in order to expose a fresh surface.The charge must be gradually raised during the first12 hours to an incipient red heat; by the 24th hourthe charge and the walls of the furnace must be at acherry-red heat, and by the 36th hour at a lively red.The effect of rabbling is not only to expose new sur-faces, but also to break up any masses which tend toagglutinate.

The coarse metal is the only solid product of thisoperation; the sulphur passes off in the form of sul-phurous and sulphuric acids,.while a proportion ofoxygen combines with the matt nearly equal to thatof the sulphur expelled. Omitting the sulphuric acid,the following tables will show the difference betweenthe substances before and after the operation :—Substances Employed.

Coarse metal. 0.804

Oxygen of the atmosphere. 0.196

Products.

Calcined coarse metal, for Op. IV. 0.5361

„ „ „ V. 0.247 i

Sulphurous acid...

1.000

The product of this operation may be bad eitherfrom the result of too high or too low a temperature.There is not much chance of too high a temperaturebeing produced, for this would agglutinate the charge,and give the workman much extra labour in rabbling.The danger is the other way, and in order to keepthe men to their work 4 inspectors are appointed to15 furnaces, whose duty it is to see that the heat isgradually and properly raised, and that the rabblingsare attended to every two hours.

The physical and chemical properties of the coarsemetal are greatly altered by calcination: the fragmentsare much reduced in size, the general colour is a deepblack, with light brown reflections; many of the grainsare friable; others are encased in a friable envelope,the nucleus being hard and compact; this, when broken,has a lustre of various colours; other fragments areformed by the incipient fusion of several particlestogether.

Pourth Operation. —White metal, the object ofthis operation, is produced by associating with thecalcined coarse metal those ores of copper which arealmost entirely free from sulpliuret of iron, and consist

F f 2

1.000

0.783

0.217